Chemical Composition(%):

t=65mm,Chemical Composition(%)
Grade C Si Mn p S N
EN 10027-1 EN 10027-2 t=40 40<t=65
S235JRH 1.0039 0.17 0.20 1.40 0.045 0.045 0.009
S275J0H 1.0149 0.20 0.22 1.50 0.040 0.040 0.009
S275J2H 1.0138 0.20 0.22 1.50 0.035 0.035
S355J0H 1.0547 0.22 0.22 0.55 1.60 0.040 0.040 0.009
S355J2H 1.0576 0.22 0.22 0.55 1.60 0.035 0.035

 

Melting analysis CEV(max.)
Grade CEV  (%)  max.
EN 10027-1 EN 10027-2 t=16 16<t=40 40<t=65
S235JRH 1.0039 0.37 0.39 0.41
S275J0H 1.0149 0.41 0.43 0.45
S275J2H 1.0138 0.41 0.43 0.45
S355J0H 1.0547 0.45 0.47 0.50
S355J2H 1.0576 0.45 0.47 0.50

Mechanical Properties:

Grade Yield Strength        
 (N/mm2) min.
Tensile Strength
(N/mm2)
Elongation
%
Impact
(J)
EN 10027-1 EN 10027-2 t=16 16<t=40 40<t=65 t=3 3<t=65 t=40 40<t=65 t=40 40<t=65 temperature Min
longitudinal transverse ? (Ave)
S235JRH 1.0039 235 225 215 360~510 340~470 26 25 24 23 20 27
S275J0H 1.0149 275 265 255 430~580 410~560 22 21 20 19 2 27
S275J2H 1.0138 -20 27
S355J0H 1.0547 355 345 335 510~680 490~630 22 21 20 19 0 27
S355J2H 1.0576 -20 27